[技术资料] shore硬度换算表,供大家参考
P:2007-04-15 16:46:35
1
| A 100 | B 85 | C 77 | D 58 | O | OO |
| 95 | 81 | 70 | 46 | | |
| 90 | 76 | 59 | 39 | | |
| 85 | 71 | 52 | 33 | | |
| 80 | 66 | 47 | 29 | 84 | 96 |
| 75 | 62 | 42 | 25 | 79 | 97 |
| 70 | 56 | 37 | 22 | 75 | 95 |
| 65 | 51 | 32 | 19 | 72 | 94 |
| 60 | 47 | 28 | 16 | 69 | 93 |
| 55 | 42 | 24 | 14 | 65 | 91 |
| 50 | 37 | 20 | 12 | 61 | 90 |
high voltage cable - 高压电缆 (0) 投诉
P:2007-04-15 16:47:56
2
| A 45 | B 32 | C 17 | D 10 | O 57 | OO 88 |
| 40 | 27 | 14 | 8 | 53 | 86 |
| 35 | 22 | 12 | 7 | 48 | 83 |
| 30 | 17 | 9 | 6 | 42 | 80 |
| 25 | 12 | | | 35 | 76 |
| 20 | 6 | | | 28 | 70 |
| 15 | | | | 21 | 62 |
| 10 | | | | 14 | 55 |
| 5 | | | | 8 | 45 |
optical pulse propagation - 光脉冲传播 (0) 投诉
P:2007-04-16 10:04:18
3
我们公司自己配的料之硬度和你给出的底2度
pin mixing screw - 轴销式混料螺杆 (0) 投诉
P:2007-04-16 11:09:53
4
请教楼主,维氏硬度应如何换算
MTS - multiplex timing source复用定时信源 (0) 投诉
P:2007-05-15 08:14:05
5
可以查询五金手册,上面有哦!
melt pressure - (挤塑)熔料压力,熔体压力 (0) 投诉
5